Informe-tecnico-final-de-pruebas-metalurgicas-para-aarl-8 (1).pdf

  • Uploaded by: Hector Suarez Rios
  • 0
  • 0
  • May 2020
  • PDF

This document was uploaded by user and they confirmed that they have the permission to share it. If you are author or own the copyright of this book, please report to us by using this DMCA report form. Report DMCA


Overview

Download & View Informe-tecnico-final-de-pruebas-metalurgicas-para-aarl-8 (1).pdf as PDF for free.

More details

  • Words: 7,427
  • Pages: 56
Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 Lima, Viernes 12 de junio del 2015 Srs. Águila American Resources Limited S.A. Calle Roca de Vergallo 158 Magdalena Del Mar Att: Ing. Rolando Dávila Gerente de Proyectos Sr. Jimy Parodi Gerente de Logística Águila American Resources Limited S.A.

INFORME TECNICO FINAL DE PRUEBAS DE LIXIVIACION POR CIANURACION-CIP A ESCALA DE LABORATORIO CON MINERAL DEL PROYECTO AURIFERO DE AGUILA AMERICAN RESOURCES LIMITED S.A.

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 Lima, viernes 12 de junio del 2015 Srs. Águila American Resources Limited S.A. Calle Roca de Vergallo 158 Magdalena Del Mar Att: Ing. Rolando Dávila Gerente de Proyectos Sr. Jimy Parodi Gerente de Logística Águila American Resources Limited S.A.

INFORME TECNICO FINAL DE PRUEBAS DE LIXIVIACION POR CIANURACION –CIP A ESCALA DE LABORATORIO CON MINERAL DEL PROYECTO AURIFERO DE AGUILA AMERICAN RESOURCES LIMITED S.A. De nuestra consideración En atención al requerimiento solicitado se está remitiendo el informe técnico final de las pruebas metalúrgicas de tratamiento de minerales de oro y plata vía los procesos de lixiviación por cianuracion-CIP a escala de laboratorio con mineral del proyecto aurífero de Águila American Resources Limited S.A, en concordancia con los descrito en la propuesta técnica –cotización N 0 131-2015-IBEROMETEX. Muy Cordialmente:

Julio Tremolada Payano. Director Gerente Instituto Iberoamericano de Metalurgia Extractiva S.A.C. Calle Marcahuasi, Mz. E’1- Lt 2, 3 Era Etapa, Urbanización Portada del Sol La Molina – Lima 12 Teléfonos: 3657308 / 97 9559936 / 948 315 123 E Mail: [email protected] / [email protected]

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 PRUEBAS DE LIXIVIACION POR CIANURACION-CIP A LABORATORIO CON MINERAL DEL PROYECTO AURIFERO AMERICAN RESOURCES LIMITED S.A.

ESCALA DE DE AGUILA

ANTECEDENTES El día Jueves 21 de mayo del presente año se dio inicio al desarrollo de los estudios metalúrgicos, según el programa de pruebas metalúrgicas elaborado para Aguila American Resources Limited S.A. para lo cual se recepciono 02 sacos de mineral fresco en el laboratorio químico metalúrgico de K.W. química Germana S.A., ubicado en el parque industrial de Chorrillos, donde se están ejecutando las correspondientes pruebas metalúrgicas. JUSTIFICACION DE LAS PRUEBAS METALURGICAS Los resultados técnicos de las presentes pruebas metalúrgicas servirán de base para los correspondientes estudios de la Ingeniería de diseño de la futura planta de procesamiento de 350 TMD de lixiviación de minerales de oro y plata. 1. RECEPCION Y PESAJE DE MUESTRAS RECEPCIONADAS. Los 02 sacos del mineral fresco de American Águila Resources cianuracion presentaron un peso total húmedo de 104.00 kilos. Dichas muestras son la base para la ejecución de los estudios metalúrgicos de lixiviación por Cianuracion CIP provenientes de la región de Abancay. CARACTERIZACION DEL MINERAL. Humedad del mineral aurífero fresco: 1.80 % Densidad aparente del mineral: 1.24 gr / ml Gravedad especifica del mineral: 2.79 pH natural del mineral: 7.27 WI Bond del mineral: Resultados pruebas WI Bond Test KW-2488-1 KW-2488-2

Feed Mass g 458.4 458.9

Final BWI kWh/mt kWh/mt 11.1 -11.1 --

GPR_150_250 Bond Wi St. BWI % 1.04 1.04

kWh/mt 11.1 11.1

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 LEYES DE CABEZA EXPERIMENTAL DEL MINERAL DE AGUILA AMERICAN RESOURCES LIMITED S.A. Au ( Onz / T.C.) : 0.9227 Onz / T.C. = 31.63 gr / TM Ag ( Onz / T.C.) : 1.3063 Onz / T.C. = 44.79 gr / TM Cu ( % ) : 0.06 Fe ( % ) : 27.97 S ( %) : 0.54 As ( % ) : 2.6 Sb ( ppm ) : 60 Hg ( ppm ) : <1 Carbon Total ( % ) : 0.08 Carbon Organico ( % ) : 0.07 ANALISIS POR ICP DEL MINERAL DE CABEZA

Ag ( ppm ) : 46 Al ( ppm ) : 2947 As ( % ) : > 10 Ba ( ppm ) : 219 Be ( ppm ) : < 0.5 Bi ( ppm ) : 60 Ca ( % ) : 1.4 Cd ( ppm ) : 2 Ce ( ppm ) : < 10 Co ( ppm ) : 5 Cr ( ppm ) : 34 Cu ( ppm ) : 626 Fe ( % ) : > 20 Ga ( ppm ) : < 10 Ge ( ppm ) : < 5 Hg ( ppm ) : < 1 In ( ppm ) : < 10 K ( % ) : 0.1 Mg ( ppm ) : 703 Mn ( ppm ) : 4550 Mo ( ppm ) : 14 Na ( ppm ) : 92 Ni ( ppm ) : 3 P ( ppm ) : 1261 Pb ( ppm ) : 1342 S ( ppm ) : 5220 Sb ( ppm ) : 57 Sc ( ppm ) : < 1 Se ( ppm ) : < 5 Sn ( ppm ) : < 10 Sr ( ppm ) : 53 Te ( ppm ) : 11 Ti ( ppm ) : 35 Tl ( ppm ) : < 5 V ( ppm ) : 137 W ( ppm ) : < 10 Zn ( ppm ) : 60

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 ANALISIS GRANULOMETRICO DE ALIMENTACION Y DESCARGA DEL MOLINO TEST WI (TEST 1)

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 ANALISIS GRANULOMETRICO DE ALIMENTACION Y DESCARGA DEL MOLINO TEST WI (TEST 2)

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 CURVA DE MOLIENDABILIDAD DEL MINERAL

Compañía :

Minera Aguila American Resources

Proyecto:

-

Muestra :

Moliendabilidad

Operador :

Ing. H. Donaires

Indice de Moliendabilidad de la Muestra de Cabeza Malla Tyler

Abertura micras

+200M - 200M

74

Total

15

Tiempo : minutos 25 Porcentaje en Peso

40

Tiempo : minutos / Peso: g 15 25 40

29.7 70.3

17.0 83.0

8.1 91.9

297.2 702.8

170.3 829.7

80.8 919.2

100.0

100.0

100.0

1000.0

1000.0

1000.0

TIEMPO PESO% 15 70.3 25.0 83.0 40.0 91.9

100.0

% PESO ACUMULADO PASANTE

90.0 80.0

70.0

% -200M y = 0.8426x + 59.263 R² = 0.954

60.0

24.7

minutos

80 % -200M

50.0 40.0 30.0

20.0

Tiempo VS Peso Acumulado Pasante

10.0 0.0

0

5

10

15

20

25

30

35

40

45

TIEMPO

Molienda Muestra : Agua : Solidos :

1000 g 500 cc 67 %

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

ANALISIS GRANULOMETRICO VALORADO DE AGUILA AMERICAN RESOURCES

Malla Nº +3/4 +1/2 +1/4 +m10 +m20 +m65 +m100 +m140 +m200

Tamaño (micras) Peso del mineral Malla promedio kg 21997 47.292 19050 15554 8.213 12700 8980 12.296 6350 2588 2000 13.505 1673 1400 7.003 1091 850 10.680 357 150 0.796 126 106 1.096 89 75 0.767

-m200 Peso Total :

--

--

% 45.37 7.88 11.80 12.96 6.72 10.25 0.76 1.05 0.74

2.583

2.48

104.231

100.00

Leyes (ppm) % Acumul. % Passing Au(onz/TC) Ag(onz/TC) 45.37 54.63 0.5201 1.397 53.25 46.75 0.9956 1.468 65.05 34.95 1.2241 1.257 78.01 21.99 1.2435 1.237 84.72 15.28 1.1356 1.237 94.97 5.03 1.0879 1.075 95.73 4.27 1.0121 0.085 96.79 3.21 0.8886 0.998 97.52 2.48 0.9625 1.047 100.00

0.00

Leyes calculadas:

Au onz 0.02460 0.00818 0.01505 0.01679 0.00795 0.01162 0.00081 0.00097 0.00074

% 27.56 9.16 16.86 18.82 8.91 13.02 0.90 1.09 0.83

Ag onz 0.0661 0.0121 0.0155 0.0167 0.0087 0.0115 0.0001 0.0011 0.0008

%

0.9849

1.188

0.00254

2.85

0.0031

48.78 8.90 11.41 12.33 6.40 8.47 0.05 0.81 0.59 2.27

0.8563

1.30

0.0893

100.00

0.1355

100.00

60.00

50.00 % de distribucion de Au, Ag

40.00

1.5749 1.1428 14.5672

30.00 51.10052832 37.08024875 472.6596076 20.00 5141.8404

10.00

0.00

+3/4

+1/2

+1/4

+m10

+m20

+m65

+m100

+m140

+m200

-m200

MALLAS

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

PRUEBAS METALURGICAS DE CIANURACION SOBRE EL MINERAL AURIFERO DE AGUILA AMERICAN RESOURCES LIMITED

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 PRUEBAS DE CIANURACION EN TANQUES AGITADORES. 1. TESTS DE CIANURACION VIA AGITACION CON VARIACION DE LA CONCENTRACION DE CIANURO Y VARIACION DE TAMAÑO DE PARTICULA. Se realizó dos test metalúrgicos de lixiviación vía agitación a granulometrías independientes de 80% < 200 mallas y 100% < 325 mallas equivalente a ( 80 % < 400 mallas), a una concentración constante cianuro de 1500 ppm ( 0.15% ) con el mineral composito fresco con el objetivo de cuantificar la disolución y recuperación metalúrgica del oro y plata soluble asociado a la roca mineral. Condiciones Experimentales Test b1: Peso de mineral compositado : 1000 gramos Volumen de agua : 2.0 litros Dilución (L / S) :2/1 Tiempo de Agitación : 12-24-66-90 horas Concentración CN: 1500 ppm pH natural del mineral : 7.27 pH de trabajo : 10.50 Granulometría mineral : 80.00 % < 200 mallas RESULTADOS Ley Au( 90 hrs en la solución) : 14.6 ppm Ley Ag (90 hrs en la solución) : 8.6 ppm Recuperación Au ( X soluciones) : 94.85% Recuperación Ag ( X soluciones) : 39.57% Recuperación Au ( X Cabeza calculada) : 91.70% Recuperación Ag ( X Cabeza calculada) : 34.90% Consumo de reactivos Cal ( kg / TM ) : NaCN ( Kg / TM ) :

8.50 Kg/ TM 8.83 Kg/TM

Condiciones Experimentales Test b2: Peso de mineral compositado Volumen de Agua Dilución ( L / S ) Granulometría Mineral Concentración CNpH de trabajo Tiempo de agitación

: 1000 gr : 2.0 litros :2 / 1 : 100%< 325 mallas ( 80 % < 400 mallas ) : 1500 ppm : 10.40 : 12-24-66-90 horas

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 RESULTADOS Ley Au( 90 hrs en la solución) Ley Ag (90 hrs en la solución) Recuperación Au ( X soluciones) Recuperación Ag ( X soluciones) Recuperación Au ( X Cabeza calculada) Recuperación Ag ( X Cabeza calculada)

: 11.00 ppm : 9.00 ppm : 71.74% : 41.50% : 89.40% : 36.10%

Consumo de reactivos Cal (kg / TM): 8.50 Kg/ TM NaCN (Kg / TM): 9.52 Kg/TM

TESTS DE CIANURACION VIA AGITACION CON VARIACION DE LA CONCENTRACION DE CIANURO  TEST DE CIANURACION VIA AGITACION CON VARIACION DE LA CONCENTRACION DE CIANURO Condiciones Experimentales (Test b3 ): Peso de mineral compositado : 1000 gramos Volumen de agua : 2.0 litros Dilución (L / S) :2/1 Tiempo de Agitación : 12-24-66-90 horas Concentración CN : 1500 ppm pH natural del mineral : 7.27 pH de trabajo : 10.50 Granulometría mineral : 80.00 % < 200 mallas RESULTADOS Ley Au (90 hrs en la solución) : 11.00 ppm Ley Ag (90 hrs en la solución) : 9.00 ppm Recuperación Au (X soluciones) : 84.02% Recuperación Ag (X soluciones) : 41.36% Recuperación Au (X Cabeza calculada) : 86.60% Recuperación Ag (X Cabeza calculada) : 35.20%

Consumo de reactivos Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Cal (kg / TM): NaCN (Kg / TM):

8.50 Kg/ TM 11.96 Kg/TM

Condiciones Experimentales (Test b4): Peso de mineral compositado : 500 gramos Volumen de agua : 1.0 litros Dilución (L / S) :2/1 Tiempo de Agitación : 8 horas Concentración CN : 5000 ppm pH natural del mineral : 7.27 pH de trabajo : 10.40 Granulometría mineral : 80.00 % < 200 mallas RESULTADOS Ley Au( 08 hrs en la solución) : 14.20 ppm Ley Ag (08 hrs en la solución) : 7.92 ppm Recuperación Au ( X soluciones) : 84.02% Recuperación Ag ( X soluciones) : 41.36% Recuperación Au ( X Cabeza calculada) : 86.60% Recuperación Ag ( X Cabeza calculada) : 35.20%

Consumo de reactivos Cal ( kg / TM ) : NaCN ( Kg / TM ) :

2.82 Kg/ TM 2.98 Kg/TM

BALANCES METALURGICOS DE RECUPERACION METALURGICA DE LOS TEST B1-B2-B3-B4

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 FECHA

29-may-15

HORA INICIO

09:00 a. m.

REPORTE DE LABORATORIO METALURGICO MUESTRA No.

B1

PRUEBA No.

1500 ppm CN-

DESCRIPCION

TK 1

80% < 200M

MALLA

Solucion Cianurada a 1500 ppm CN PRODUCTO

PESO

ENSAYES g/t

g

Au

Ag

CABEZA ENSAYADA

31.63 44.79

RESIDUO ENSAYADO

2.700

33.00

* CABEZA CALCULADA

32.70

50.72

RESIDUO ENSAYADO

2.70

33.00

EXTRACCION %

mg Au mg Ag

Au

Ag

91.5

26.3

91.7

34.9

Hg

DETALLES EXPERIMENTALES CONDICIONES INICIALES PRUEBA

Condiciones de Prueba

PESO

VOL

Kg

L

1.000

2.000

L/S

CN- NaCN ppm

2.00

g

1500 3.046

CONDICIONES FINALES pH

CaO

pH

Inicial

g

Final

7.27

CONSUMO Kg/t

Factor

8.50 10.50

-

NaCN

CaO

8.83

8.50

mg Totales Au

Ag

31.63

44.79

CONTROL DE LA PRUEBA NaCN g

Cabeza

TIEMPO

pH

Horas

Inicio Ajustado

ml Reman Agreg

Agreg

Au

Ag

Au

Ag

0

7.27

10.50

-

-

3.046

8.500

-

-

0.00

0.00

H

12

10.40

10.47

0.42

0.35

2.302

0.000 9.000 6.530

56.91

29.16

12

9.00

24

10.47

10.88

1.22

0.61

1.807

0.000 9.800 7.660

62.68

34.57

48

9.800

66

10.88

10.95

0.46

0.38

2.274

0.000 13.300 7.960

85.58

36.30

66

90

10.95

10.95

1.20

0.60

-

0.000 14.600 8.600

94.85

39.57

90

AgNO3

ENSAYES ppm

CaO g

EXTRACCION %

PROCEDIMIENTO Acondicionamiento de pH 10.50

Ag

31.63

44.79

Ley Soluciones

Extracciones

Pérdida en

Au

Ag

6.53

56.91

29.16

Au

7.66

61.97

34.20

0.23

13.300

7.96

84.10

35.54

0.47

14.600

8.60

92.32

38.40

0.80

Reales

25 mL

Au

Ag

Ag

56.91

29.16

0.16

62.68

34.57

0.34

85.58

36.30

0.52

94.85

39.57

30.0025 17.72251

CINETICA DE RECUPERACION (B1) MALLA 80% <200m CONCENTRACION DE CIANURO 1500ppm

32.7025 50.72251

8.83

2.7 CABEZA CALCULADA

100 % EXTRAC C C IO N

BALANCE Extracciones

8.50

Condiciones finales de Prueba COMENTARIOS

Tiempo

Au

33

32.7025 50.7225

80 TIEMPO

60 40

EXTRACCION %

Horas

Au

Ag

72 HORAS

87.89

37.12

20

INTERPOLACION

0 0

10

20

30

40

50 Au Ag

60

70

80

90

TIEMPO (h)

100

x2 = ((y2 - y1)(x3 - x1) / (y3 - y1)) + x1 EXTRACION % (Au) X1 = 85.58 X2 = X X3= 94.85 X2 = 87.89

Y1 = 66 Y2 = 72 Y3 = 90

EXTRACION % (Ag) X1 = 34.57 Y1 = 66 X2 = X Y2 = 72 X3=39.57 Y3 = 90 X2 = 37.12

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 FECHA

29-may-15

HORA INICIO

09:00 a. m.

REPORTE DE LABORATORIO METALURGICO MUESTRA No.

B2

PRUEBA No.

1500 ppm CN-

DESCRIPCION

TK 2

100% < 325m (80% <400m)

MALLA

Solucion Cianurada a 1500 ppm CN PRODUCTO

PESO

ENSAYES g/t

g

Au

Ag

CABEZA ENSAYADA

31.63

44.79

RESIDUO ENSAYADO

2.700

32.90

* CABEZA CALCULADA

25.39

51.49

RESIDUO ENSAYADO

2.70

32.90

EXTRACCION %

mg Au mg Ag

Au

Ag

91.5

26.5

89.4

36.1

Hg

DETALLES EXPERIMENTALES CONDICIONES INICIALES PRUEBA

Condiciones de Prueba

PESO

VOL

Kg

L

1.000

2.000

L/S

CN- NaCN ppm

2.00

g

1500 3.046

CONDICIONES FINALES pH

CaO

pH

Inicial

g

Final

7.27

7.92 10.40

CONSUMO Kg/t

Factor -

NaCN

CaO

9.52

8.50

mg Totales Au

Ag

31.63

44.79

CONTROL DE LA PRUEBA NaCN g

Cabeza

TIEMPO

pH

Horas

Inicio Ajustado

ml Reman Agreg

Agreg

Au

Ag

Au

Ag

0

7.92

10.40

-

-

3.046

8.500

-

-

0.00

0.00

H

12

10.20

10.29

0.24

0.20

2.559

0.000 8.600

7.000

55.06

31.26

12

24

10.29

10.76

1.16

0.58

1.868

0.000 8.900

7.280

57.66

32.90

66

10.76

10.81

0.26

0.22

2.605

0.000 10.200 7.720

65.88

35.27

90

10.81

11.00

1.12

0.56

-

0.000 11.000 9.000

71.74

41.50

AgNO3

ENSAYES ppm

CaO g

EXTRACCION %

PROCEDIMIENTO Acondicionamiento de pH 10.50

Condiciones finales de Prueba

9.52

COMENTARIOS

Ag

31.63

44.79

Ley Soluciones

BALANCE Extracciones

Extracciones

Pérdida en

Au

Ag

Reales

25 mL

Au

Ag

8.600

7.000

54.38

31.26

Au

Ag

54.38

31.26

24

8.900

7.280

56.28

32.51

0.22

0.18

56.96

32.90

66

10.200

7.720

64.50

34.47

0.44

0.36

65.88

35.27

90

11.000

9.000

69.55

40.19

0.69

0.59

71.74

41.50

22.6925 18.5886

8.50

2.7

CINETICA DE RECUPERACION (B2) MALLA 100%<325m(80%<400m) CONCENTRACION DE CIANURO 1500ppm

100 % EXTRAC C C IO N

Tiempo

Au

32.9

25.3925 51.4886 CABEZA CALCULADA

25.3925 51.4886

80 60 TIEMPO

40

Horas

EXTRACCION % Au

Ag

72 HORAS 67.35

20

36.83

0 0

10

20

30

40

50 Au

60 Ag

70

80

90

100

INTERPOLACION

TIEMPO (h)

x2 = ((y2 - y1)(x3 - x1) / (y3 - y1)) + x1 EXTRACION % (Au) X1 = 65.88 Y1 = 66 X2 = X Y2 = 72 X3= 71.74 Y3 = 90

EXTRACION % (Ag) X1 = 35.27 Y1 = 66 X2 = X Y2 = 72 X3=41.50 Y3 = 90

X2 = 67.35

X2 = 36.83

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 FECHA

29-may-15

HORA INICIO

09:00 a. m.

REPORTE DE LABORATORIO METALURGICO MUESTRA No.

B3

PRUEBA No.

2000 ppm CN-

DESCRIPCION

TK 3

80% < 200m

MALLA

Solucion Cianurada a 2000 ppm CN PRODUCTO

PESO

ENSAYES g/t

g

Au

Ag

CABEZA ENSAYADA

31.63

44.79

RESIDUO ENSAYADO

4.100

34.10

* CABEZA CALCULADA

30.68

52.63

RESIDUO ENSAYADO

4.10

34.10

EXTRACCION %

mg Au mg Ag

Au

Ag

87.0

23.9

86.6

35.2

Hg

DETALLES EXPERIMENTALES CONDICIONES INICIALES PRUEBA

Condiciones de Prueba

PESO

VOL

Kg

L

1.000

2.000

L/S

CN- NaCN ppm

2.00

g

2000 4.061

CONDICIONES FINALES pH

CaO

pH

Inicial

g

Final

7.27

6.97 10.40

CONSUMO Kg/t

Factor -

NaCN

CaO

11.96

8.50

mg Totales Au

Ag

31.63

44.79

CONTROL DE LA PRUEBA NaCN g

Cabeza

TIEMPO

pH

Horas

Inicio Ajustado

ml Reman Agreg

Agreg

Au

Ag

Au

Ag

0

7.92

10.40

-

-

4.061

8.500

-

-

0.00

0.00

H

12

10.40

10.57

0.32

0.26

3.470

0.000 9.100

6.450

57.54

28.80

12

24

10.57

11.10

2.08

1.04

1.949

0.000 9.900

6.860

63.32

30.99

66

11.10

11.10

0.34

0.28

3.486

0.000 12.000 7.730

77.38

35.26

90

11.10

11.20

2.02

1.01

-

0.000 12.900 9.000

84.02

41.36

AgNO3

ENSAYES ppm

CaO g

EXTRACCION %

PROCEDIMIENTO Acondicionamiento de pH 10.50

Condiciones finales de Prueba

11.96

COMENTARIOS

Tiempo

Au

Ag

31.63

44.79

Ley Soluciones

BALANCE Extracciones Au

Ag

Reales

25 mL

Au

Ag

9.100

6.450

57.54

28.80

Au

Ag

57.54

28.80

24

9.900

6.860

62.60

30.63

0.23

0.16

63.32

30.99

66

12.000

7.730

75.88

34.52

0.48

0.33

77.38

35.26

90

12.900

9.000

81.57

40.19

0.78

0.53

84.02

41.36

26.575

18.526

8.50

CINETICA DE RECUPERACION ( B3) MALLA 80%<200m CONCENTRACION DE CIANURO 2000 ppm CABEZA CALCULADA

100 % EXTRAC C C IO N

Extracciones

Pérdida en

4.1

34.1

30.675

52.626

30.675 52.626

80 TIEMPO

60 40

EXTRACCION %

Horas

Au

Ag

72 HORAS

79.04

36.79

20 0 0

10

20

30

40

50 Au

60 Ag

70

80

90

TIEMPO (h)

INTERPOLACION

100

x2 = ((y2 - y1)(x3 - x1) / (y3 - y1)) + x1 EXTRACION % (Au) X1 = 77.38 Y1 = 66 X2 = X Y2 = 72 X3= 84.02 Y3 = 90

EXTRACION % (Ag) X1 = 35.26 Y1 = 66 X2 = X Y2 = 72 X3= 41.36 Y3 = 90

X2 = 79.04

X2 = 36.79

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

FECHA

30-may-15

HORA INICIO

09:00 a. m.

REPORTE DE LABORATORIO METALURGICO MUESTRA No.

B4

PRUEBA No.

5000 ppm CN-

DESCRIPCION

TK 4

80% < 200m

MALLA

Solucion Cianurada a 5000 ppm CN PRODUCTO

PESO

ENSAYES g/t

g

Au

Ag

CABEZA ENSAYADA

31.63

44.79

RESIDUO ENSAYADO

4.500

33.20

* CABEZA CALCULADA

33.70

49.44

RESIDUO ENSAYADO

4.50

33.20

EXTRACCION %

mg Au

mg Ag

Au

Ag

Hg

85.8

25.9

86.6

32.8

DETALLES EXPERIMENTALES CONDICIONES INICIALES PRUEBA

PESO Kg

L

Condiciones de Prueba

0.500

1.000

PROCEDIMIENTO Acondicionamiento de pH 10.50

VOL

L/S

CN-

2.00

pH

TIEMPO

CONDICIONES FINALES NaCN

pH

ppm

g

Inicial

g

Final

5000

5.076

7.27

2.82

10.40

AgNO3

CONTROL DE LA PRUEBA NaCN g

CaO

CONSUMO Kg/t

Factor -

NaCN

CaO

5.95

5.64

mg Totales Au

Ag

15.815

22.395 Cabeza

ENSAYES ppm

CaO g

Horas

Inicio

Ajustado

ml

Reman

Agreg

Agreg

0

7.92

10.40

-

-

5.076

2.820

8

10.40

10.65

4.02

2.10

-

0.000

2.98

2.82

Condiciones finales de Prueba

pH

Au

Ag

14.200

7.920

EXTRACCION % Au

Ag

Tiempo

0.00

0.00

H

89.79

35.37

12

Au

Ag

31.63

44.79

Ley Soluciones 16.200

7.920

BALANCE Extracciones Au

Ag

89.79

35.37

COMENTARIOS

CINETICA DE RECUPERACION (B4) MALLA 80%<200m CONCENTRACION DE CIANURO 5000 ppm

Extracciones

Pérdida en

CABEZA CALCULADA

Reales

25 mL Au

Ag

14.6 2.25 16.85 33.7

Au

Ag

89.79

35.37

8.12 16.6 24.72 49.44

100.00 90.00 % EXTRACCION

80.00

70.00 60.00

oro

50.00

plata

40.00

30.00 20.00 10.00 0.00

0

TIEMPO (horas)

8

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

RESUMEN DE PRUEBAS DE EXTRACCION DE ORO Y PLATA

MUESTRA

MALLA

Conc. CNNa LIXIVIACION (ppm)

TIEMPO

B1 B2 B3 B4

80% < 200m 100%<325m (80%<400m) 80% < 200m 80% < 200m

1500 1500 2000 5000

90 Horas 90 Horas 90 Horas 8 Horas

% EXTRACCION % EXTRACCION % EXTRACCION % EXTRACCION SOLIDO Au SOLIDO Ag SOLUCION Au SOLUCION Ag

91.50 91.50 87.00 85.80

26.30 26.50 23.90 25.90

94.85 71.74 84.02 89.79

34.57 41.5 41.36 35.37

CURVAS CINETICAS DE RECUPERACION DE ORO Y PLATA

CINETICA DE RECUPERACION (B1) MALLA 80% <200m CONCENTRACION DE CIANURO 1500ppm

80

80

% EXTRAC C C IO N

100

% EXTRAC C C IO N

100

60 40

20

CINETICA DE RECUPERACION (B2) MALLA 100%<325m(80%<400m) CONCENTRACION DE CIANURO 1500ppm

60 40

20

0

0 0

10

20

30

40

50

60

Au

70

80

90

100

0

10

20

30

TIEMPO (h)

Ag

40

50 Au

60

70

80

90

100

TIEMPO (h)

Ag

CINETICA DE RECUPERACION (B4) MALLA 80%<200m CONCENTRACION DE CIANURO 5000 ppm

CINETICA DE RECUPERACION ( B3) MALLA 80%<200m CONCENTRACION DE CIANURO 2000 ppm

100.00

100

80.00 % EXTRACCION

% EXTRAC C C IO N

90.00 80 60

40 20

70.00 60.00

oro

50.00

plata

40.00 30.00

20.00

0 0

10

20

30

40

50 Au

60 Ag

70

80

90

TIEMPO (h)

100

10.00 0.00

0

TIEMPO (horas)

8

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

BALANCE COSTO BENEFICIO EN EL CONSUMO DE CIANURO (Kg/ t) MUESTRA

MALLA

% EXTRACCION SOLIDO Au

B1 B2 B3 B4

80% < 200m 100%<325m (80%<400m) 80% < 200m 80% < 200m

91.50 91.50 87.00 85.80

Conc. CNNa

% EXTRACCION LIXIVIACION SOLIDO Ag (ppm)

26.30 26.50 23.90 25.90

1500 1500 2000 5000

CONSUMO (kg/t)

COSTO EN $DOLARES

NaCN

CaO

NaCN (2.2 $ /kg)

CaO ( 0.1$/kg)

8.83 9.52 11.96 5.95

8.5 8.5 8.5 5.64

19.426 20.944 26.312 13.09

0.85 0.85 0.85 0.564

PRUEBAS METALURGICAS DE ADSORCION DE ORO –PLATA SOBRE CARBON ACTIVADO A PARTIR DE PULPAS CIANURADAS-PROCESO CIP DEL MINERAL AURIFERO DE AGUILA AMERICAN RESOURCES LIMITED

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 BALANCE DE RECUPERACION EN EL SISTEMA DE ADSORCION CON CARBON ACTIVADO ( PROCESO CIP )

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 CAPACIDAD DE CARGA DE Au y Ag EN EL CARBON ACTIVADO ( PROCESO CIP )

Test

Código

Descripción

Conc. CNNa ADSORCION (ppm)

1 2 3

B1- carbón cargado B2 - carbón cargado B4 - carbón cargado

3 horas 3 horas 1 hora

600 560 2100

Peso CARBON CARGADO (gr)

Ley de Au en el carbon (g/kg)

Ley de Ag en el carbón (g/kg)

54.5 54.6 35.8

0.4002 0.3161 0.4924

0.2212 0.2326 0.2056

TIEMPO DE RESIDENCIA DE ADSORCION Y CAPACIDAD DE CARGA DE Au-Ag PROYECTADA EN EL CARBON ACTIVADO ( PROCESO CIP )

TIEMPO DE ADSORCION Y CAPACIDAD DE CARGA PROYECTADA MALLA 80 % < 200m

Código

TIEMPO (minutos)

B4 B4 B4 B4 B4 B4 B4 B4 B4 B4 B4

0 10 15 30 45 60 75 90 105 107 120

1 hora 47 min

Ley Final en Ley Final en adsorcion adsorcion Ley de Au en el Soluc. Au Soluc. Ag Soluciones Au Soluciones Ag carbon (g/kg) (ppm) (ppm) (%) (%)

14.200 4.64 4.09 3.14 2.55 2.18 1.41 0.78 0.14 0.00 0.00

7.920 3.05 2.78 2.24 1.90 1.69 1.25 0.89 0.53 0.17 0.00

CALCULOS PROYECTADOS

-

32.65 28.82 22.11 17.96 15.35 9.92 5.46 1.01 0 0

38.51 35.10 28.28 23.99 21.34 15.78 11.22 6.67 2.11 0.00

0 0.0821 0.1231 0.1231 0.2462 0.4924 0.6155 0.7386 0.8617 0.8781 0.9848

Ley de Ag en el carbon (g/kg)

0 0.0343 0.0514 0.1028 0.1542 0.2056 0.2570 0.3084 0.3598 0.3667 0.4112

DATOS REALES DATOS CALCULADOS CON LAS PROYECTADOS

INTERPOLACION x2 = ((y2 - y1)(x3 - x1) / (y3 - y1)) + x1 Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

TIEMPO DE ADSORCION Y CAPACIDAD DE CARGA PROYECTADA MALLA 80 % < 200m 35.00 30.00

% ADSORCION

% ADSORCION

25.00 20.00 15.00

Au

10.00 5.00 0.00 0

10

20

30

40

50

60

70

TIEMPO minutos

45.00 40.00

% ADSORCION

35.00 30.00 25.00 20.00

Ag

15.00 10.00 5.00 0.00 10

15

30

45

60

TIEMPO minutos

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 ANALISIS POR ICP DE LA SOLUCION PREGNANT PROVENIENTE DE LA CIANURACION EN TANQUES AGITADORES

Ag ( ppm ) : 12 Al ( ppm ) : 1 As ( ppm ) : 537 Ba ( ppm ) : < 1 Be ( ppm ) : < 0.5 Bi ( ppm ) : < 2 Ca ( ppm ) : 4 Cd ( ppm ) : 0.1 Ce ( ppm ) : < 10 Co ( ppm ) : < 1 Cr ( ppm ) : < 1 Cu ( ppm ) : 72 Fe ( ppm ) : 37 Ga ( ppm ) : < 10 Ge ( ppm ) : < 5 Hg ( ppm ) : < 0.5 In ( ppm ) : < 10 K ( ppm ) : 47 Mg ( ppm ) : < 0.01 Mn ( ppm ) : < 2 Mo ( ppm ) : 1.03 Na ( ppm ) : > 50 Ni ( ppm ) : 0.2 P ( ppm ) : 1 Pb ( ppm ) : < 2 S ( ppm ) : 952 Sb ( ppm ) : 0.2 Sc ( ppm ) : < 1 Se ( ppm ) : 0.5 Sn ( ppm ) : < 10 Sr ( ppm ) : 0.01 Te ( ppm ) : < 5 Ti ( ppm ) : < 1 Tl ( ppm ) : < 5 V ( ppm ) : 0.5 W ( ppm ) : 0.10 Zn ( ppm ) : 4

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

CANTIDAD DE OXIGENO DISUELTO (PPM) EN LOS TANQUES AGITADORES La concentracion de oxigeno disuelto depende principalmente del contenido de oxigeno de la fase gas en contacto con la pulpa o solucion lixiviada,temperature y altitud. La concentracion de oxigeno disponible en la mayoria de operaciones de lixiviacion del oro varian de 5 mg /L a una altitud de 2000 msnm y a 8.2 mg/L a nivel del mar.

CANTIDAD DE AIRE EN LOS TANQUES AGITADORES La cantidad teorica que se require para saturar una pulpa tipica es 0.02 a 0.04 kg/T de mineral. La aplicacion practica requerira de un volumen de aire de 0.16 Pie 3 / gal pulpa.

EFECTO DE PULPAS SATURADAS CON OXIGENO SOBRE LA ADSORCION CON CARBON ACTIVADO La practica industrial en diferentes operaciones mineras a cielo abierto y en mineria subterraneana ha demostrado y ha podido establecer que para disoluciones saturadas en oxigeno (arriba de 8 ppm) se producira una mayor adsorcion del oro en el carbon activado en relacion a disoluciones de bajo contenido de oxigeno .Siendo este efecto mas importante para disoluciones de baja fuerza ionica y en menor grado para disoluciones de elevada fuerza ionica.

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

CONCLUSIONES Y RECOMENDACIONES

1 ) Las diferentes concentraciones de cianuro evaluadas a 1500 ppm,2000 ppm y 5000 ppm nos permiten afirmar en funcion a los resultados obtenidos que la velocidad maxima de extraccion del oro es obtenida a una concentracion de cianuro de 1500 ppm y a un tamaño de particular adecuado de 80% < 200 mallas, donde se consiguieron obtener extracciones de oro de 91.7% y de plata de 34.9 %, esto es para un tiempo de residencia de 90 horas de lixiviacion por cianuracion en tanques ( ver test b1). A las 72 horas de lixiviacion la extraccion del oro esta en el orden de 87.89 %.El consumo de cianuro obtenido en este test es del orden de 8.83 kg /t y de cal de 8.5 kg/t. 2 ) Incrementar la molienda mas fina a 100 % < 325 mallas equivalente a 80% < 400 mallas no tiene efecto en conseguir mayor extraccion de oro, siendo la recuperacion obtenida al cabo de 90 horas de 89.4% y de 36.1% de plata ( ver test b2). A las 72 horas de lixiviacion la extraccion del oro esta en el orden de 67.35 %. 3 ) Concentraciones elevadas de cianuro com 2000 ppm y 5000 ppm no tienen ningun efecto en incrementar la extraccion de los metals preciosos oro y plata ( ver test b3 y b4). 4 ) El balance costo beneficio en el consumo de cianuro es mostrado en los archivos en excel que se adjuntan al presente informe tecnico. 5 ) El tiempo de adsorcion y la capacidad de carga en los carbones activados marca calgon de tamaño 6 x 12 son mostrados :

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

TIEMPO DE ADSORCION Y CAPACIDAD DE CARGA PROYECTADA MALLA 80 % < 200m

Código

TIEMPO (minutos)

B4 B4 B4 B4 B4 B4 B4 B4 B4 B4 B4

0 10 15 30 45 60 75 90 105 107 120

1 hora 47 min

Ley Final en Ley Final en adsorcion adsorcion Soluc. Au Soluc. Ag Soluciones Au Soluciones Ag (ppm) (ppm) (%) (%)

14.200 4.64 4.09 3.14 2.55 2.18 1.41 0.78 0.14 0.00 0.00

7.920 3.05 2.78 2.24 1.90 1.69 1.25 0.89 0.53 0.17 0.00

-

32.65 28.82 22.11 17.96 15.35 9.92 5.46 1.01 0 0

38.51 35.10 28.28 23.99 21.34 15.78 11.22 6.67 2.11 0.00

Ley de Au en el carbon (g/kg)

Ley de Ag en el carbon (g/kg)

0 0.0821 0.1231 0.1231 0.2462 0.4924 0.6155 0.7386 0.8617 0.8781 0.9848

0 0.0343 0.0514 0.1028 0.1542 0.2056 0.2570 0.3084 0.3598 0.3667 0.4112

6 ) El tiempo de residencia en los tanques CIP esta en el orden de 2 horas y la capacidad de carga del oro y la plata en los carbones activados cargados son del orden del 0.9848 gr Au /kg carbon ( 0.98 kg Au / TM carbon ) y de 0.4112 gr Ag / kg carbon ( 0.4112 kg Au / TM carbon ) para el citado tiempo de residencia. 7 ) Podemos afirmar categoricamente que segun los analisis quimicos reportados por TCM del mineral de Aguila American Resources Limited, por laboratorio externo de reconocido prestigio internacional, los resultados de TCM con codigo AMRL-IBEROMETEX indican lo siguiente: TCM % Carbon Total :0.08 % Carbon Organico :0.07

Por tanto el mineral puede utilizar la tecnologia del proceso carbon en pulpa ( CIP) sin ningun tipo de problema hipotetico por efecto preg robbing asociado a la roca mineral, esta conclusion es especifica para este tipo de mineral que ha sido evaluado. Tener en consideracion que concentraciones de Carbon organico mayores de 0.1% podran generar problemas en la extraccion de los metals preciosos oro y plata por Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 tanto el TCM debera ser una variable de control en la calidad de mineral que se alimentara a la futura planta de 350 TMD. 8 ) El work index del mineral presenta el valor de 11.1 Kwh / mt catalogandose como un mineral de dureza blanda. 9 ) Concentraciones de oxigeno disuelto arriba de 5 ppm seran requeridos en los tanques agitadores de la futura planta que estara ubicada en abancay que esta por arriba de lo 4000 msnm. Por Tanto la cantidad de oxigeno disuelto requerida como la cantidad de aire necesaria para los tanques agitadores debera ser sumistrado a traves de compresora y / o de blowers.

10 ) En la prueba de analisis granulometrico valorado por oro y plata se ha evidenciado la presencia de oro grueso, hecho que nos permite sugerir que el diseño de ingenieria de la futura planta de 350 TMD se considere una etapa de gravimetria a la descarga del Molino. 11 ) Los analisis quimicos del mineral de cabeza muestran presencia de arsenico en el orden de magnitud del 2.6%, y de > 10% en analisis por ICP, y en valores de 537 ppm en la solucion rica de cianuracion, a este compuesto se le puede atribuir el consumo de cianuro de sodio. 12) La relacion Ag / Au obtenida (44.79 gr / ton / 31.63 gr / ton = 1.42) hace factible la aplicacion del proceso CIP pra arecuperar los metales una vez disueltos, dado que cuando dicha relacion es demasiada alta (mayor de 12) tal proceso no es recomendable por la competencia de la Plata con el oro por su gran adsorcion sobre el carbon, lo que se hace necesite de grandes cantidades de carbon para recuperar pequeñas cantidades de oro, lo cual no es rentable economicamente.

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

CIANURACION EN TANQUES AGITADORES

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

ANEXOS

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 ANALISIS GRANULOMETRICO MINERAL AGUILA AMERICAN RESOURCES LIMITED

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 CIANURACION EN TANQUES AGITADORES TEST B1 B2 B3

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 CIANURACION EN TANQUE AGITADOR B4

PROCESO CIP

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 COMPRESORA DE AIRE PARA TEST CIP

PESO DE CARBON ACTIVADO PARA TEST CIP

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 TESTS DE MOLIENDABILIDAD EN MOLINO DE BOLAS

LIMPIEZA DEL MOLINO DE BOLAS

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 TAMIZADO POR 200 MALLAS- TEST DE MOLIENDABILIDAD

MOLIENDABILIDAD DE MINERALES

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 TUBO DISPERSADOR DE AIRE. PROCESO CIP

FILTRACION DE PULPAS DE CIANURACION TEST B1 B2

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Instituto Iberoamericano De Metalurgia Extractiva S.A.C IBEROMETEX S.AC Consultora Minera Metalurgia Ambiental Teléfono: (511) 3657308 Móvil: (5176) 976390590 TUBOS DE MUESTRAS DE SOLUCIONES PREGNANTS DE CIANURACION PARA LECTURA POR ABSORCION ATOMICA

CARGA DE BOLSA EN MOLINO- TEST MOLIENDABILIDAD

Iberometex SAC Calle Marcahuasi Mz. E1 Lt 2, 3ra Etapa, Urb. Portada Del Sol La Molina, Lima 12, Perú www.iberometex.com

Related Documents

Chile 1pdf
December 2019 139
Theevravadham 1pdf
April 2020 103
Majalla Karman 1pdf
April 2020 93
Rincon De Agus 1pdf
May 2020 84
Exemple Tema 1pdf
June 2020 78

More Documents from "Gerardo Garay Robles"