Long Term Testing on Keratherm Materials 0-Probe : this is the material right after production 100 h TWB: 100 h cycle test (one cycle from –40 to +95 °C in 1 hour) 100 h 95%, 95°C: 100 hours at 95% humidity and 95°C 100 h at 150 °C: self explaining 500 h at 150 °C: self explaining 1000 h at 150 °C: self explaining

Thermal aging on Keratherm 86/17 (0,225 mm) 9 8 0,6 7 0,5 6 0,4 5 4 Rth [K/W] 0,3 3 0,2 2 Ud [kV] 0,1 1 0 0 0-Probe 100h TWB 100h 95% 100h 150° 500h 150° 1000h 95° 150°

Dielectric Breakdown Ud [kV]

Thermal Resistance Rth [K/W]

0,7

Test method

0,36 0,34 0,32 0,3 0,28 0,26 0,24 0,22 0,2 0-Probe

Rth [K/W] Ud [kV]

100h TWB

100h 95% 100h 150° 500h 150° 95° Test method

1,8 1,6 1,4 1,2 1 0,8 0,6 0,4 0,2 0 1000h 150°

Dielectric Breakdown Ud [kV]

Thermal Resistance Rth [K/W]

Thermal aging on Keratherm 86/30 (0,225 mm)

0,55

10

0,54

9

0,53

8

0,52

7

0,51

6

0,5

5

0,49

Rth [K/W]

0,48

3 Ud [kV]

0,47 0,46 0,45 0-Probe

4 2 1

100h TWB

100h 95% 95°

100h 150°

Dielectric Breakdown Ud [kV]

Thermal Resistance Rth [K/W]

Thermal aging on Keratherm 86/37 (0,225 mm)

0 500h 150° 1000h 150°

Test method

Thermal aging Keratherm 86/50 (0,225 mm) 2

0,18

1,8

0,16

1,6

0,14

1,4

0,12

1,2

0,1

Rth [K/W]

0,08 0,06

Ud [kV]

1 0,8 0,6

0,04

0,4

0,02

0,2

0 0-Probe

100h TWB

100h 95% 95°

100h 150°

Test method

500h 150°

0 1000h 150°

Dielectric Breakdown Ud [kV]

Thermal Resistance Rth [K/W]

0,2

0,98

7

0,96

6 5

0,94

4 0,92 3 0,9

Rth [K/W]

2

0,88

1

Ud [kV] 0,86 0-Probe

100h TWB

100h 95% 95°

100h 150°

500h 150°

Dielectric Breakdown Ud [kV]

Thermal Resistance Rth [K/W]

Thermal aging Keratherm 86/77 (0,3 mm)

0 1000h 150°

Test method

Thermal aging on Keratherm 86/200 12

2,25 10 2,2 2,15

8

2,1 6 2,05

Rth [K/W]

2

4

1,95

Ud [kV]

1,9 1,85 0-Probe

100h TWB

100h 95% 95°

100h 150°

Test method

500h 150°

2

Dielectric Breakdown Ud [kV]

Thermal Resistance Rth [K/W]

2,3

0 1000h 150°

1,5 1,45 1,4 1,35 1,3 1,25 500 h - 85/85

100 h - 85/85

500 h - TWB

1000 h - 150°C

500 h - 150°C

250 h - 150°C

100 h - 150°C

1,2 Ausgangsprobe

Thermal Conductivity [W/mK]

Aging Test Softtherm 86/255 [0,5 mm]

Thermal aging on Keratherm Graphite 0,160

Thermal Resistance [K/W]

0,140 0,120 0,100

90/20 90/10

0,080

90/10-S 90/15

0,060 0,040 0,020 0,000 0-Probe

100 h / 120 °

500 h / 120 ° Test Method

1000 h / 120 °

150 h - 95/95-Test

Long Term Life Test for Softtherm 86/200 Specimen was stored for about 8 – 10 years and tested for thermal and electrical performance

Longterm Life Test Softtherm 86/200 (20-22°C, 45-55 % humidity)

Thermal Resistance [K/W]

2,5

2,25

Softtherm 86/200 2

1,75 1

100

1000

5000

10000

Test tim e in hours

Longterm Life Test Softtherm 86/200 (20-22 °C, 45-55 % humidity) 9

Dieelectric Breakdown [kV]

8 7 6 5 Softtherm 86/200 4 3 2 1 0 1

100

1000 Testtim e in hours

5000

10000

Related Documents

Heat Sinks
November 2019 9
Heat Sinks
October 2019 14
Installing Sinks
May 2020 6
Installing Sinks
November 2019 13
Heat
October 2019 71